Titanium grade 4 plate hot rolling, annealing and pickling

November 24, 2026

Grade 4 occupies an unusual position in the titanium family. It is still commercially pure titanium — no aluminium, no vanadium — yet its elevated oxygen and iron content push minimum yield strength to 480 MPa, comfortably above many stainless steels, while retaining the corrosion immunity that makes CP titanium the default choice in chloride and oxidising service. That combination makes it a favourite for medical implant hardware, aerospace brackets, heat-exchanger components, cryogenic vessels and high-strength marine fittings. But it also makes the production route unforgiving: the same interstitial oxygen that delivers the strength narrows the hot-working window, raises rolling loads and makes surface conditioning after hot work absolutely essential. Hot rolling, annealing and pickling are therefore not three separate processing steps but one continuous metallurgical argument. Drawing on more than twenty years of titanium production at Jucheng Titanium — Baoji Jucheng Titanium Industry Co., Ltd., located in China's Titanium Valley — this article walks through how each stage shapes the final properties, surface quality and fabrication behaviour of titanium grade 4 plate, and what buyers should specify to get what they actually need.

Jucheng plant & Ti plate​​​​​​​​

 

Why Grade 4 Behaves Differently From Grades 1 and 2

The Interstitial Chemistry Behind the Strength

Grade 4 titanium is unalloyed titanium that allows for up to 0.40% oxygen and up to 0.50% iron. This is almost twice as much oxygen as Grade 2, which allows for maximum oxygen content. By occupying interstitial spaces in the hexagonal alpha lattice, oxygen is able to impede the migration of dislocations and significantly increase the strength of the material without the addition of any alloying. The material that is produced as a consequence has a minimum tensile strength of 550 MPa and a minimum yield of 480 MPa, while at the same time being completely alpha-phase and resistant to corrosion in the same settings in which Grade 2 performance is exceptional. As a result of this, titanium grade 4 plate is more resistant to deformation than lesser grades, it work-hardens more quickly, and it can endure a smaller temperature range during hot work before cracking or excessive oxygen pick-up becomes an issue. This is a practical consequence for processing.

 α-Ti lattice oxygen schematic​​​​​​​​

 

Comparative Position Within the CP Titanium Family

PropertyGrade 1Grade 2Grade 3Grade 4
Max oxygen0.18%0.25%0.35%0.40%
Max iron0.20%0.30%0.30%0.50%
Min tensile strength240 MPa345 MPa450 MPa550 MPa
Min yield strength (0.2%)170 MPa275 MPa380 MPa480 MPa
Min elongation24%20%18%15%
Relative formabilityHighestHighModerateModerate
Typical hardness~120 HV~145 HV~180 HV~220 HV
Density4.51 g/cm³4.51 g/cm³4.51 g/cm³4.51 g/cm³
UNS designationR50250R50400R50550R50700

CP Ti Gr1-4 property chart​​​​​​​​


Where the Grade Earns Its Place

In situations when they want a higher level of strength than Grade 2 can provide, but do not wish to deal with the financial burden, weldability issues, or biocompatibility concerns that are connected with Ti-6Al-4V, specifiers opt for Grade 4. As a result of the fact that unalloyed titanium completely circumvents any argument about vanadium release, dental and orthopaedic implant components provide a significant outlet. Airframe fittings, cryogenic tanks, hydraulic tubing flanges, naval fasteners, and chemical-process components that need a wall thickness that is as thin as possible all adhere to the same rationale. Buyers of titanium grade 4 plate often request complete traceability, ultrasonic testing, and strict control of the delivery condition. Jucheng Titanium incorporates these requirements into its regular paperwork package rather than considering them as extras. This is because the material is subjected to rigorous service.

Grade 4 Ti application samples (medical, heat exchanger, marine)​​​​​​​​

 

Hot Rolling: Establishing Microstructure and Dimension

Ingot Preparation and Breakdown

VAR or double-VAR melted ingot is the starting point for production. After being conditioned, the ingot is then forged or broken down in the beta field, which is located above the beta transus. The beta transus temperature for Grade 4 is around 950 degrees Celsius, depending on the particular interstitial content. When beta-field working is performed, the coarse as-cast structure is effectively broken apart. This is due to the fact that the body-centered cubic beta phase deforms far more easily than alpha. Following this, the slab is warmed and finish-rolled in the alpha-beta or high alpha region, generally at temperatures ranging from 760 to 900 degrees Celsius, in order to generate a fine, equiaxed aluminium grain structure. The production of titanium grade 4 plate with consistent characteristics throughout thickness is dependent on the successful completion of this transition. An excessive amount of beta-field finishing results in a coarsely converted structure that has decreased ductility, while finishing that is too cold increases the likelihood of edge cracking.

Titanium ingot, cogging & hot rolling slab​​​​​​​

 

Rolling Schedule, Temperature Control and Distortion

Titanium has a poor thermal conductivity, which means that a plate loses heat from its surface much more quickly than it loses heat from its core. This results in a temperature gradient, which in turn causes uneven deformation and residual stress. Mills with more experience are able to do this by reducing rolling speeds on heavier gauges, carefully graded reduction schedules, and controlled warming between passes. Because of the greater flow stress in Grade 4, mill loads are increased by a significant margin in comparison to Grade 2, which results in pass reductions that are typically lower and pass counts that are higher. The process of pack rolling, in which a number of thin plates are rolled together inside of a steel envelope, continues to be a typical method for thin gauges since it simultaneously reduces the amount of heat loss and oxygen exposure. Later on, the quality of this stage manifests itself in the form of flatness, thickness uniformity, and the amount of residual stress that a fabricator must struggle with during cutting.

Alpha Case Formation — The Unavoidable Consequence

Above roughly 550 °C, titanium absorbs oxygen aggressively from the furnace atmosphere, forming a hard, oxygen-enriched surface layer known as alpha case. It is brittle; it cracks under forming strain; it initiates fatigue failures; and it compromises weld quality. Hot rolling always produces it; the only question is how deep. On heavy titanium grade 4 plate sections with long soak times, alpha case may extend several tenths of a millimetre beneath the scale. This is precisely why pickling is not cosmetic finishing but a mandatory metallurgical operation, and why plate sold as "hot rolled, as-is" should be treated with suspicion for any application involving forming, welding or fatigue loading.

Metallograph of alpha case cross-section​​​​​​

 

Annealing: Relieving Stress and Fixing Properties

Standard Mill Annealing Parameters

Mill-annealed is the standard method of delivery for grade 4. After maintaining temperatures between 650 and 760 degrees Celsius for a period of time that is proportionate to the thickness of the material (about one hour for every 25 millimetres, with a practical minimum), the heat is then cooled by air. Because it is a single-phase alpha, Grade 4 cannot be reinforced by heat treatment in the same way as Ti-6Al-4V can. Annealing helps to recrystallise the structure that has been treated, alleviate rolling stresses, restore ductility, and offer uniform and predictable mechanical characteristics. However, air annealing is permitted in situations where a subsequent pickling operation would remove the ensuing scale and contaminated layer from the surface of the titanium grade 4 plate. Vacuum or inert-atmosphere annealing is preferable for higher-specification work because it restricts additional oxygen pick-up.

Vacuum annealing furnace for titanium plate ​​​​​

 

Stress Relief Versus Full Anneal

These are different operations serving different purposes, and confusing them causes real problems. Stress relief is performed at lower temperatures — roughly 480 °C to 595 °C — for shorter times, and is used after welding, machining, or forming to reduce residual stress without altering grain structure or hardness. Full annealing recrystallises the material and resets mechanical properties. Fabricators building large assemblies often need post-weld stress relief to prevent distortion during subsequent machining, but must avoid temperatures that would soften the plate below specification. If you are unsure which treatment your fabrication sequence requires, send your drawing and process route to s4@juchengti.com — the Jucheng Titanium technical team will advise on the appropriate thermal cycle, delivery condition and surface specification before you place the order.

Annealing Reference Conditions

TreatmentTemperature RangeTypical HoldCoolingPurpose
Mill anneal650 – 760 °C1 h per 25 mmAirStandard delivery condition
Vacuum anneal700 – 760 °C1 – 2 hFurnace/inert gasClean surface, no alpha case growth
Stress relief480 – 595 °C1 – 4 hAirPost-weld / post-machining relief
Recrystallisation anneal760 – 800 °C1 – 2 hAir or vacuumMaximum ductility restoration
Beta anneal (rare for Gr 4)Above beta transusShortControlledSpecific toughness requirements

Atmosphere, Fixturing and Flatness Control

On the annealing floor, there are two practical difficulties that predominate. First, the atmosphere: furnaces that were once used for steel may transmit hydrogen and impurities, and hydrogen pick-up that is more than 0.015% causes embrittlement that cannot be reversed by any amount of pickling. Dedicated furnaces or furnaces that have been completely cleaned are required. Second, fixturing: a thin plate will deform under its own weight when it is heated to the annealing temperature, and uneven support will generate waviness that will need to be addressed later by roller levelling or stretch straightening, both of which will reintroduce stress. Support spacing, loading density, and heating rates are all carefully managed by mills that produce high-quality titanium grade 4 plate. In order to achieve this level of process discipline throughout the manufacture of both plate and fabricated equipment, Jucheng Titanium's facility, which spans 120,000 square meters, and its dedicated quality inspection staff are both very important.

Pickling: Removing Scale and Alpha Case

Descaling Before Acid Treatment

Pickling begins with mechanical or chemical descaling. Shot blasting or molten salt bath descaling removes the tenacious oxide scale formed during hot rolling and annealing, exposing the metal for acid attack. Molten caustic or salt-bath treatment is particularly effective on heavy scale and is widely used ahead of acid pickling on thick sections. Attempting to pickle heavily scaled plate directly wastes acid, produces uneven attack and leaves patches of residual alpha case — the worst possible outcome, since the plate looks finished but carries embrittled regions. For titanium grade 4 plate with its typically deeper alpha case, thorough descaling before acid immersion is not optional.

Nitric–Hydrofluoric Acid Chemistry and Hydrogen Control

A combination of nitric acid and hydrofluoric acid, typically in the range of 15–30% HNO3 and 1–3% HF, is usually used as the standard pickling medium. This mixture is kept at a temperature that is under control. A significant amount of importance is placed on the ratio: hydrofluoric acid is responsible for dissolving, while nitric acid functions as an oxidiser, which prevents hydrogen from being absorbed into the metal. Hydrogen embrittlement is produced when there is an insufficient amount of nitric acid in comparison to the amount of hydrogen fluoride (HF) and atomic hydrogen that is created at the surface. This embrittlement will not become apparent until the component breaks while it is being used. The acid concentrations, titanium loading in the bath, and temperature are continually monitored by pickling lines that are operating efficiently. Additionally, the hydrogen content of the completed plate is verified by analysis. This is one of the most obvious technical distinctions that can be made between a legitimate producer and a dealer who is reselling goods that have not been validated.

Titanium pickling line & in-line inspection ​​​​

 

Verifying Complete Alpha Case Removal

Rather than being presumed, removal must be proven. Metallographic cross-section examination under a microscope, in which the alpha case appears as a distinct featureless white layer; microhardness traverse from the surface inward, in which elevated near-surface hardness betrays residual case; and bend testing, in which cracking at the outer fibre indicates a remaining brittle layer are the verification methods that are most commonly used. It is also important to verify the dimensions since pickling eliminates material, generally between 0.05 and 0.15 millimetres per side, and extensive pickling on thin gauges might cause the thickness to fall below the tolerance levels. Prior to the release of titanium grade 4 plate, the quality inspection team at Jucheng Titanium checks the surface condition in addition to the chemical, mechanical characteristics, and ultrasonic findings.

Final Surface, Inspection and Documentation

StageControl ParameterVerification Method
Hot rollingFinish temperature, reduction scheduleProcess records, thickness gauging
DescalingScale removal completenessVisual, surface roughness
AnnealingTemperature, time, atmosphereFurnace charts, hardness
PicklingHNO₃:HF ratio, bath temperature, timeBath titration, logs
Alpha case removalDepth of removalMetallography, microhardness, bend test
Hydrogen content≤ 0.015%Inert gas fusion analysis
Internal soundnessDiscontinuity detectionUltrasonic per ASTM B600 / agreed class
DimensionsThickness, flatness, widthMeasurement against ASTM B265
CertificationHeat number, chemistry, mechanicalsEN 10204 3.1 certificate

UT & metallurgical lab inspection of Ti plate​​​​


Choosing a Producer Who Controls All Three StagesWhy Integrated Processing Matters

A flaw that is created at any one step cannot be repaired at any subsequent stage. Hot rolling is responsible for determining the microstructure, annealing is responsible for fixing characteristics, and pickling is responsible for restoring surface integrity. When suppliers outsource annealing or pickling, they lose insight into the characteristics that are most important to each individual manufacturer. Baoji Jucheng Titanium Industry Co., Ltd. was established in 2004 and is the first private titanium enterprise in Shaanxi Province to list on the National Equities Exchange and Quotations. The company is the owner of four invention patents and forty-one utility model patents, all of which are applied in production. Additionally, the company is recognised as a National High-Tech Enterprise and a national-level specialised "little giant" enterprise. Collaboration with the Northwest Institute for Nonferrous Metal Research, Tsinghua University, and Northwest University serves as the foundation for the ongoing process development.

Capability, Stock and Customisation

In addition to plates, Jucheng Titanium manufactures 1,500 tonnes of titanium anode plates per year, with a market share of more than 70 percent in the hydrometallurgy industry. Additionally, the company manufactures more than 500 sets of titanium equipment every year, which includes heat exchangers, reactors, and air coolers, and it has an almost 90 percent market share in the coking sector. Its composite tubes made of titanium have been commissioned at Luoyang Petrochemical; the WUGANG Group is served by the biggest titanium spiral plate heat exchanger in China, and all-titanium air coolers have been approved in North America. A comprehensive after-sales management staff and collaborations with companies such as Jiangxi Copper Group are in place to enable the provision of a standard service that includes tailored manufacturing and processing to client specifications. Additionally, an inventory of around 3,000 tonnes of titanium is kept on hand throughout the year for the purpose of expedited shipment.

Conclusion

The strength of titanium grade 4 plate comes from interstitial oxygen, which also makes processing demanding. Controlled hot rolling, correct annealing and properly balanced nitric–HF pickling together determine properties, surface integrity and fabrication behaviour. Specify all three explicitly, and verify them.

FAQ

1. Why is Grade 4 stronger than Grade 2?

Higher permitted oxygen and iron content strengthens the alpha lattice interstitially — no alloying elements are involved.

2. What is alpha case and why must it be removed?

A brittle oxygen-enriched surface layer formed during hot work; it cracks during forming and initiates fatigue failures.

3. Can Grade 4 be strengthened by heat treatment?

No. It is single-phase alpha, so annealing only relieves stress and restores ductility rather than increasing strength.

4. What acids are used for pickling?

A controlled nitric–hydrofluoric mixture, with the nitric ratio maintained high enough to suppress hydrogen absorption.

Specify Your Grade 4 Plate With Jucheng Titanium

Need annealed, pickled titanium grade 4 plate with verified alpha case removal and full mill certification? Send your thickness, dimensions, condition and drawing for a fast quotation. With 3,000 tonnes in stock and 20 years of expertise, Jucheng Titanium delivers. Email s4@juchengti.com today.

Jucheng Titanium​​​​

 

References

1. ASTM International. ASTM B265: Standard Specification for Titanium and Titanium Alloy Strip, Sheet, and Plate.

2. Donachie, M. J. Titanium: A Technical Guide, 2nd Edition. ASM International, 2000.

3. Lütjering, G., & Williams, J. C. Titanium, 2nd Edition. Springer, 2007.

4. Boyer, R., Welsch, G., & Collings, E. W. (Eds.). Materials Properties Handbook: Titanium Alloys. ASM International, 1994.

5. ASM International. ASM Handbook, Volume 4: Heat Treating — Heat Treating of Titanium and Titanium Alloys.

6. ASTM International. ASTM B600: Standard Guide for Descaling and Cleaning Titanium and Titanium Alloy Surfaces.

Online Message